Dr Vijesh Vijayan, the Anti Corrosion Experts FZ LLC
Introduction
- Field Context and Failure Question
Water ballast tanks combine several conditions that challenge protective coatings: seawater immersion, concentrated chlorides, alternating wet and dry periods, condensation, restricted drainage and complex steel geometry. The coating is expected to isolate the steel throughout these exposures and to support the long-term protection objective of the International Maritime Organisation, (IMO) performance standard for dedicated seawater ballast tanks [1]. System selection also needs to reflect the immersion environment and durability principles in ISO 12944-5 [2], while also considering mechanical impacts. In maintenance work, surface-tolerant epoxy mastics are attractive because they can be applied to steel that cannot be fully abrasive blasted during a short dry-docking period. Their tolerance of marginal preparation does not, however, make them insensitive to strain.
A rigid, high-build epoxy can crack or detach when the underlying plate bends, particularly where coating spot repairs over an existing film have produced excessive and discontinuous thickness. These coating repairs must not be confused with welded-steel repairs. This article examines a field case in which coating breakdown inside a water ballast tank was concentrated opposite an external hull belt showing abrasion, gouging and other evidence consistent with repeated tug and fender contact. The investigation combined visual inspection, photographic mapping, coating-failure classification and ultrasonic thickness measurements. The purpose was to distinguish the initiating event from the conditions that accelerated deterioration after the barrier had been breached.
Figure 1. External Shell Condition in The Tug-Contact Belt: (a) Extensive Abrasion and Mechanical Scarring; (b) Longitudinal Scraping and Coating Loss Near the Splash Zone
2. Field Evidence and Diagnostic Approach
The inspection was completed during scheduled dry-docking. External damage was mapped against internal stiffeners, brackets, existing welds and shell plating. Inside the tank, deterioration was most severe at stiffener toes, bracket intersections, weld heat-affected zones, lower drainage paths and shell areas aligned with the external contact belt. The welds were structural reference locations and stress-concentration features, importantly the investigation did not identify weld repair as the cause.
These locations are susceptible because local plate flexure, geometric discontinuity, moisture retention and difficult coating access can act together.
Observed defects were classified using the ISO 4628 series [3]. Rusting reached approximately Ri4-Ri5 in the worst areas; cracking was consistent with Cr3; and flaking was typically Fl3-Fl4. The photographs showed sharply defined lifted edges, radial or transverse cracking near welds, rust blooming beneath semi-adherent film and localised pits after coating loss. These patterns are more consistent with a coating barrier opened by movement than with uniform chemical degradation alone. Three visual zones were particularly informative. Below the internal waterline, shell plating opposite the tug-contact belt showed the broadest coating loss and the deepest corrosion craters. Around stiffeners and brackets, the coating detached at toes and corners, leaving curled edges and bare steel. In low points and drainage paths, rust spread beneath apparently intact film and pits formed where saline water could remain. The distribution explains why neither impact nor immersion alone is a complete diagnosis: panel impact (restrained by the stiffeners and/or brackets) created preferential entry points, while the ballast-tank microclimate controlled the subsequent corrosion rate.
Figure 2. Internal Deterioration: (a) Rust Clusters and Underfilm Propagation Around Weld Penetrations, (b) Coating Loss and Pitting at A Lower Girder Corner.
The sequence inferred from the survey was:
- Local hull contact produced elastic or plastic deflection of shell plating and connected members;
- The epoxy, especially where overbuilt, developed microcracks or lost adhesion under flexural and interfacial shear strain;
- Seawater, oxygen and chlorides entered through the damaged film;
- Differential aeration, condensation and retained saline water drove underfilm corrosion; and
- Continued exposure produced pitting, undercutting and further
Adhesive and cohesive failures were both present. Adhesive failure occurred at the steel–coating interface, commonly at marginally prepared or contaminated surfaces. Cohesive cracking occurred within the epoxy film, most visibly in overbuilt coating patches that had become too rigid to follow the plate. These modes then interacted: a cohesive crack admitted electrolyte, corrosion products generated wedging stress, and the adjacent weak interface detached. At existing edges and weld toes, geometry concentrated mechanical strain and moisture ingress.
Table 1 condenses the visual evidence and its diagnostic significance. The classification identifies the observed appearance; it does not by itself prove the initiating load. The spatial match between the external impact belt and internal failures provides the important supporting evidence.
Table 1. Observed Failure Modes and Diagnostic Interpretation.
Figure 3. Later-Stage Internal Damage: (a) Stratified Corrosion and Severe Delamination Following Moisture Ingress; (b) Cracking and Blistered Rust Nodules in A Stress-Affected Area.
3. Mechanical Loading, Coating Overbuild and Steel Loss
A screening estimate illustrates the scale of energy available during controlled contact. For a tug displacement of 450,000 kg and a contact speed of approximately 0.5 m/s, the kinetic energy is:
E = ½mv² = ½ × 450,000 × 0.5² = 56.25 kJ
Not all of this energy is transferred to the vessel, and the calculation is not a substitute for a berth-energy or structural analysis. It nevertheless shows why a nominally slow manoeuvre can impose a meaningful, highly localised load. Transfer through the shell can distort plating, stiffeners and brackets and place a comparatively brittle coating in bending and shear.
The critical coating condition was excessive dry film thickness in previous coating spot repairs, the product being composed of a two-component, high-solids, surface-tolerant epoxy mastic with a nominal recommended film of 250-320 µm. Recorded local thickness of approximately 800-900 µm was about 2.5-3.6 times that nominal range, depending on the comparison point, because additional coating had been applied over existing full coats. ISO 19840 provides procedures for measuring and accepting dry film thickness [4], while SSPC-PA 2 provides a further method for assessing conformance [5]. The available field records did not demonstrate comparable control.
Excessive thickness reduced the ability of the cured film to accommodate substrate strain. It also created abrupt thickness transitions at repair boundaries, residual stress within the coating and a larger bending strain through the film. Under repeated flexure, these zones fractured first. Marginal adhesion then allowed the cracked coating to lift in sheets.
The root-cause hierarchy therefore separated initiation from amplification. Tug-induced deformation was the primary driver because it accounted for the location and morphology of the earliest cracking. Excessive film build was the most important coating-related amplifier because the worst failures occurred in overcoated coating-maintenance zones. Preparation and edge treatment were likely poor, soluble contamination, water retention and incomplete application control were secondary contributors. Welds and weld toes were identified where strain and coating discontinuity were concentrated. The secondary contributors do not explain the external-to-internal spatial correlation, but they explain why a mechanically opened defect progressed rapidly to widespread delamination and pitting.
Photogrammetric scaling indicated an average failed patch of about 0.35 m². Across 12 mapped patches, the estimated affected area was therefore approximately 4.2 m². The damage clustered around weld toes, brackets and shell plating behind the external contact zone rather than being uniformly distributed. Ultrasonic readings confirmed that the coating failure had progressed to measurable steel loss. Against a design thickness of 14.0 mm, the lowest recorded value was 9.1 mm on the bottom plating at an existing weld seam, equivalent to a 35.0% reduction; this identifies the measurement location. The impact-zone reading was 9.4 mm, or 32.9% reduction, and the maximum observed pit depth was approximately 2.5-3.0 mm. These readings require location-specific assessment against the vessel’s approved scantlings and class limits; the IACS (International Association of Classification Societies) requirements provide the relevant material and structural context [6].
The difference between the nearly intact mid-tank plate and the severely reduced weld and impact-zone readings is important. A uniform immersion mechanism would be expected to produce a broader distribution. Instead, the local measurements support a damage process focused at stress raisers and at positions where coating continuity had already been lost. The results also show why visual coating grades cannot replace thickness gauging: similar rust appearance can conceal very different remaining plate thicknesses.
Table 2. Ultrasonic Thickness Readings and Condition Assessment.
4. Why the Barrier Became Vulnerable
Mechanical flexure of restrained components initiated the failure, but the inspection identified several conditions that lowered resistance or accelerated corrosion.
Surface Preparation and Soluble Salts
General tank areas were reported at approximately Sa 2, while some localised and access-restricted maintenance areas relied on St 3 power-tool cleaning. This fell short of the Sa 2½ preparation used as the benchmark for the intended ballast-tank coating performance. ISO 8501-1 defines the visual preparation grades [7]. Restricted access around brackets and existing weld geometry also produced variable anchor profile, and no consistent profile verification against ISO 8503-1 was documented [8].
Soluble salts measured by the Bresle method reached 43 mg/m² [9]. This value was below the 50 mg/m² project benchmark cited from the ballast-tank performance standard but above the coating manufacturer’s stated limit of 30 mg/m². In poorly rinsed or poorly drained recesses, retained salts therefore increased the likelihood of osmotic activity and underfilm corrosion once the film was damaged. When requirements differ, the more restrictive product or project limit should govern.
The distinction between nominal compliance and product suitability is central to the case. A reading may satisfy a general project ceiling while still exceeding the threshold used to qualify the particular coating. Moreover, a spot measurement does not exclude higher concentrations in crevices, behind brackets or beneath retained corrosion products.
Cleaning acceptance should therefore combine representative salt testing with visual confirmation of drainage and access, rather than treating one numerical result as proof that the whole repair area is suitable.
Edges, Application Records and Quality Assurance
Stripe coating was inconsistent at weld toes, cut-outs and bracket edges. These geometries already have limited film build and high local stress; incomplete stripe coats left them susceptible to edge lifting and early ingress. Design and surface-finish guidance for immersion linings similarly emphasises rounded edges, accessible geometry and careful treatment of welds [10].
The available records did not establish continuous monitoring of wet and dry film thickness, relative humidity, steel temperature, dew-point margin, overcoating intervals or shop-primer compatibility. Nor did they confirm the coating-inspector qualifications and overall competency, expected by the project quality plan. The incomplete Coating Technical File limited traceability of batches, climatic conditions, preparation, adhesion tests, final thickness and repair history.
The IMO performance standard uses a nominal 15-year target coating life to the first major maintenance, whereas the reported breakdown was observed after approximately five to seven years. Its direct statutory or contractual applicability to this maintenance campaign depends on the vessel and repair scope; in this investigation it was used as a performance benchmark. Several departures could reduce the service margin: preparation below Sa 2½ in some locations, no demonstrated control of a nominal 320 µm film, local thickness above 900 µm, partially executed stripe coats and absent climatic records. Compatibility of any retained shop primer was also not documented. Each departure matters independently, but their combined effect is more damaging where structural discontinuities are simultaneously difficult to prepare, difficult to stripe coat and subject to high strain.
Table 3 compares the principal performance controls with the field evidence. The selected epoxy had suitable immersion resistance in principle; the gap arose from the combination of mechanical demand and execution outside the intended application envelope.
Table 3. Multiple Field-to-Specification Gaps Associated with Premature Failure.
5. Engineering Response
The most effective response is to treat the tug-contact belt as a combined structural and coating risk zone rather than as a series of isolated paint defects. External bumper protection could be considered at the ship design stage.
Repair Specification
Repairs should always follow ultrasonic mapping and engineering review of any location close to renewal criteria. Corrosion products, undercut film and contaminants should be removed, with abrasive preparation to Sa 2½ wherever practicable. Power-tool preparation should be restricted to genuinely inaccessible, manufacturer-approved locations. Salt testing should follow rinsing, and the acceptance value should not exceed the coating manufacturer’s limit.
The repair boundary must extend to sound, well-adhered coating. Pits and cavities require particular attention because residual salts and moisture can remain after the surrounding flat plate appears clean. Surface profile should be checked with a recognised comparator; the original recommendation was a 50-75 µm Rz anchor pattern for the high-solids epoxy. Where that profile cannot be achieved or verified, the coating manufacturer should approve a revised repair procedure before application.
In flexure-prone locations, coating selection should include evidence of mechanical compliance, not only immersion resistance. A system with elongation at break of at least 5% and improved crack-bridging capability should be considered. A flexible epoxy underlayer beneath a harder abrasion-resistant finish may be suitable where supported by product qualification and compatibility testing. The final system and thickness must remain within the manufacturer’s approved specification, with any special circumstances reported back to the manufacturer for advice.
Application Control
Repair boundaries should be feathered to avoid abrupt steps. Stripe coats are required at welds, edges, brackets, scallops and cut-outs. Wet-film readings during application and calibrated dry-film measurements after cure should be recorded for every repair area. The cumulative dry film thickness should be controlled within the approved range; repeat overcoating of sound film should not be used to conceal poor transitions.
Inspection lots should be small enough to identify a local overbuild rather than reporting only a broad tank average. Readings need to cover the centre of a repair, its feathered perimeter, welds and adjacent intact coating. Out-of-range areas should be resolved through an approved concession or corrective action, not covered by an additional coat. Recoat intervals and cure conditions must be checked against the technical data sheet because both premature and delayed overcoating can weaken intercoat adhesion.
Steel temperature, ambient humidity and dew point should be logged, maintaining at least a 3°C margin above dew point. Surface profile, soluble salts, batch numbers, mixing, induction time, recoat interval, holidays and final acceptance should be recorded in the Coating Technical File. Inspection methods and inspector competence should be verified independently before work starts.
Structural and Lifecycle Measures
The external tug-contact belt should be mapped against internal framing and incorporated into inspection plans. Where contact is recurrent, operators should review fendering, tug procedures and the feasibility of energy-dissipating or sacrificial protection. Internal details should avoid sharp edges, inaccessible recesses and abrupt terminations that concentrate strain or prevent continuous coating application.
Targeted visual and ultrasonic inspections at three- to five-year intervals are appropriate for structurally active zones, with shorter intervals where wall loss or continuing impact is found. Repeated spot repairs should trigger a full tank reassessment rather than another layer of local overbuild. Class guidance can support class-aligned coating and maintenance planning [11].
The inspection record should use fixed reference points so that photographs, coating grades, pit depth and ultrasonic readings can be compared from one campaign to the next. A zone that remains dimensionally stable may justify continued monitoring; a zone showing progressive plate loss, renewed cracking or continuing impact evidence requires structural and operational intervention. This closes the loop between coating maintenance and the cause of damage, rather than repeatedly treating only the visible symptoms.
Conclusion
The field pattern indicates a mechanically initiated coating failure amplified by application and environmental weaknesses with damage clustered around weld toes, brackets and shell plating behind the external contact zone, rather than being uniformly distributed.
External tug or fender contact was aligned with internal cracking, delamination and corrosion at structural discontinuities. Previous coating spot repairs and not welded-steel repairs had created local films of approximately 800-900 µm, reducing strain tolerance. Once flexure opened the barrier, marginal preparation, inconsistent stripe coating, chloride retention and incomplete quality records accelerated underfilm corrosion and pitting.
The practical lesson is that a surface-tolerant epoxy is not a mechanically tolerant system by default. Ballast-tank repairs in contact-prone regions must integrate structural risk mapping, verified surface preparation, product-specific salt limits, disciplined thickness control and competent inspection. Coating chemistry alone cannot compensate for repeated substrate movement or uncontrolled overbuild. Lessons learned should be incorporated into future vessel design by Naval architects.
References
- International Maritime Organization, Performance Standard for Protective Coatings for Dedicated Seawater Ballast Tanks in All Types of Ships and Double-Side Skin Spaces of Bulk Carriers, Resolution 215(82).
- ISO 12944-5:2019, Paints and Varnishes — Corrosion Protection of Steel Structures by Protective Paint Systems — Part 5: Protective Paint
- ISO 4628, Paints and Varnishes — Evaluation of Degradation of Coatings, Parts 3, 4 and 5: Rusting, Cracking and
- ISO 19840:2012, Paints and Varnishes — Corrosion Protection of Steel Structures by Protective Paint Systems — Measurement of, and Acceptance Criteria for, the Thickness of Dry Films on Rough Surfaces.
- SSPC-PA 2, Procedure for Determining Conformance to Dry Coating Thickness Requirements.
- IACS UR W11, Rev. 9, Normal and Higher Strength Hull Structural
- ISO 8501-1:2007, Preparation of Steel Substrates Before Application of Paints and Related Products — Visual Assessment of Surface Cleanliness.
- ISO 8503-1:2012, Preparation of Steel Substrates Before Application of Paints and Related Products — Surface Roughness Characteristics of Blast-Cleaned Steel Substrates — Part 1: Specifications and Definitions for ISO Surface Profile
- ISO 8502-6:2020 and ISO 8502-9:2020, Preparation of Steel Substrates Before Application of Paints and Related Products
- Tests for the Assessment of Surface Cleanliness: Extraction of Water-Soluble Contaminants and Field Conductometric Determination of Water-Soluble Salts.American Bureau of Shipping, Guidance Notes on the Inspection, Maintenance and Application of Marine Coating Systems, 2017
- NACE SP0178-2007, Design, Fabrication, and Surface Finish Practices for Tanks and Vessels to Be Lined for Immersion Service.